Technical data
|
BOND COATING: Nickel based, density of 7.0 to 7.5 gm/cc as sprayed |
|
|
Porosity |
2-10% depending on spray parameters: - We aim for the higher end for thermal barriers. |
|
Average coating weight |
0.75 kg/m² / 0.1mm (100 µm) |
|
Thermal conductivity is comparable with normal stainless steel |
|
|
Surface roughness |
12 - 20 µmRa |
|
CERAMIC COATING: Zirconium based density of 4.3gm/cc as sprayed |
|
|
Porosity |
8-12% |
|
Coating weight |
0.43 kg/m2 /0.1mm (100 µm) |
|
Thermal conductivity |
1.69 W/m K |
|
Surface roughness |
9-11 µmRa |
|
Coating thickness total |
Approx 300 - 350µm comprising ~ 100µm metal bond coat and 200-250µm ceramic. |
Our high temperature coatings may be removed by grit blasting if so required. The materials are NOT asbestos based, and NON fibrous and have no health and safety implications.